scieee AI-readable full text Open interactive document viewer

Photocatalytic removal of patent blue V dye on Au-TiO2 and Pt-TiO2 catalysts

Vaiano, Vincenzo; Sannino, Diana; Murcia Mesa, Julie Joseane; Hidalgo López, María del Carmen; Navío Santos, José Antonio; Ciambelli, P; Lervolino, Giussepina

Abstract

In this work it was studied the efficiency of a photocatalytic process for the removal of patent blue V. This dye is very difficult to remove by conventional treatments such as adsorption or coagulation therefore the photocatalytic process is a very interesting alternative for the removal this dye mainly because it does not require expensive oxidants and it can be carried out at mild temperatures and pressures. In this work it was tested the efficiency of Au-TiO2 and Pt-TiO2 photocatalysts in the Patent blue V removal. The Au-TiO2 catalysts were prepared by two different methods: chemical reduction and photochemical deposition; Pt-TiO2 catalysts were obtained only by photochemical deposition. In the synthesis of the catalysts prepared by photochemical deposition, it was evaluated the influence of some parameters, such as deposition time and the intensity of the light source over the physicochemical properties and photocatalytic activity of the materials obtained. An analysis of the effect of the catalyst dosage and initial patent blue V concentration over the dye degradation efficiency was also attempted. In general, it was observed that the presence of Au or Pt on TiO2 enhances the patent blue V photodegradation; it was found that noble metal particle size and distribution on TiO2 surface are important factors influencing the dye removal. The highest dye degradation was obtained over the Au-TiO2 catalyst prepared by photochemical deposition, using high light intensity and 15 min of deposition time during the synthesis. A discoloration and a total organic carbon (TOC) removal of 93 and 67% respectively, were obtained over this material after 180 min of UV irradiation. These values are higher than that the obtained on S-TiO2 (discoloration and TOC removal of about 25% and 3%, respectively).

Full text

Figure 1. SEM images of photocatalysts synthesized using different methods: photodeposition (PD) and chemical reduction (CR). (A) Au-TiO2(PD-HI)15min; (B) Au- TiO2(PD-HI)120min; (C) Au-TiO2(CR); (D) Pt-TiO2(PD-HI)15min and (E) Pt-TiO2(PDHI)120min. Au Au Au (A) (B) (D) (E) Pt Pt Pt Pt (C) Au Figure 2. TEM images of metallized S-TiO2. (A) and (B) Au-TiO2 catalysts prepared by PD method using 140 W/m2 of light intensity and different deposition time 15 and 120 min, respectively. (C) and (D) Pt-TiO2 samples prepared by photodeposition method and different deposition time 15 and 120 min, respectively. (C) (D) - Figure 3. XRD patterns for TiO2 and M-TiO2 photocatalysts (M=Au or Pt) prepared by chemical reduction (CR) and photochemical deposition (PD) using 120 min of deposition time. 20 30 40 50 60 70 80 Pt-TiO2 (PD) Au-TiO2 (PD) Au-TiO2 (CR) Intensity (a.u) 2 S-TiO2 Figure 4. UV-Vis DRS spectra for the investigated photocatalysts. 200 300 400 500 600 700 800 0,0 0,2 0,4 0,6 0,8 1,0 Absorbance (a.u) Wavelenght (nm) S-TiO2 Au-TiO2(PD -HI) 15min Au-TiO2(PD-HI) 120min Pt-TiO2(PD-HI) 15min Pt-TiO2(PD-HI) 120min Au-TiO2(CR) Figure 5. Discoloration of the Patent blue V as a function of run time over the photocatalysts analyzed; Patent blue V initial concentration: 7 mg/L; catalyst dosage: 3 g/L. 0 0,2 0,4 0,6 0,8 1 1,2 050 100 150 200 250 300 350 C/Co Run time [min] Au-TiO2 (CR) S-TiO2 Au-TiO2 (PD-LI) 15 min Au-TiO2 (PD-HI) 120min Au-TiO2 (PD-LI) 120 min Au-TiO2 (PD-HI)15 min UV ON Figure 6. Total Organic Carbon (TOC) removal as a function of run time over the catalysts analyzed. Patent Blue V initial concentration: 7 mg/L; catalyst dosage: 3 g/L. 0 0,2 0,4 0,6 0,8 1 1,2 050 100 150 200 250 300 350 TOC/TOCo Run time [min] S-TiO2 Au-TiO2 (CR) Au-TiO2 (PD-LI) 15 min Au-TiO2 (PD-LI) 120min Au-TiO2 (PD-HI) 120min Au-TiO2 (PD-HI) 15 min UV ON Figure 7. Patent blue V discoloration over Au-TiO2(PD-HI)15min catayst, varying the initial concentration of the dye; catalyst dosage: 3 g/L. 0 0,2 0,4 0,6 0,8 1 1,2 050 100 150 200 250 300 350 400 450 C/Co Run time (min) 7 mg/L 12 mg/L 3 mg/L UV ON Figure 8. Evaluation of Patent blue V adsorption constant on Au-TiO2(PD-HI)15min catalyst; catalyst dosage: 3 g/L. y = 751,94x + 2314,4 0 2000 4000 6000 8000 10000 12000 14000 16000 18000 20000 0 5 10 15 20 25 C0*/C* C0* Figure 9. Experimental and predicted data as a function of Patent blue V initial concentration on Au-TiO2(PD-HI)15min; catalyst dosage: 3 g/L. 0 0,2 0,4 0,6 0,8 1 1,2 050 100 150 200 C/C0* Irradiation time [min] Experimental Model 3 mg/L 12 mg/L 7 mg/L Figure 16. Evaluation of Patent blue V discoloration and mineralization after 60 minutes of irradiation on Au-TiO2(PD-HI)15min catalyst for different cycles; Patent blue V initial concentration: 4.7 mg/L; catalyst dosage: 3 g/L. 0 5 10 15 20 25 30 35 40 45 50 1 2 3 4 % discoloration and mineralization Cycle